- 1. What Compression Set Measures on a PU Bump Stop
- 2. Test Conditions: Deflection, Temperature and Time
- 3. From Report Percentage to Millimetres of Height Loss
- 4. Reading a Supplier Set Report: Four Patterns
- 5. What Drives Set: Cure, Post-Cure and Compound Identity
- 6. A Cost Model for Excess Set
- 7. Writing Compression Set into the Drawing: Field Sheet and Checklist
- 8. Frequently Asked Questions
- 8.1. Is a lower compression set value always the better part?
- 8.2. Can I compare a 24-hour result with a 70-hour result by scaling?
- 8.3. Why did hardness pass on every batch but the parts still took a set in the field?
- 8.4. We received two batches with matching hardness but clearly different set results. What does that mean?
- 8.5. Does specifying an NDI compound remove compression set concerns?
- 8.6. What set limit should I write on the drawing for a passenger car bump stop?
Compression Set in PU Bump Stops: Why 25% Beats 70 Hours
Compression set is the share of a polyurethane bump stop's deformation that never recovers after the load is removed, and it is the property that decides whether the part still has its height after a season of service. The percentage on a supplier's report, however, is meaningless without its test conditions: deflection, temperature and duration all change the number.
A buyer who compares a 6% figure from one quotation against a 4% figure from another is usually comparing two different tests. This article explains what the test measures, why the conditions behind the number matter more than the number itself, how to convert a report percentage into millimetres of lost height, and what excess set costs over a programme. It ends with a field sheet you can paste straight into a drawing.

What Compression Set Measures on a PU Bump Stop
Compression set measures how much deformation remains after a part has been held compressed and then released. In service, a jounce bumper is compressed for long periods rather than cycled endlessly, so the relevant question is how much of that compression stays in the material afterwards. The cells of cast polyurethane that have been squeezed for months adopt a new shape, and the bumper comes back shorter than it was.
A part with a high set engages late. Because the engagement point of the bumper is set by its free height, a shorter bumper lets the suspension travel further before the stop begins to work, which the driver feels as a car that no longer absorbs the same impacts. On a vehicle where the damper was valved around the bumper's support, the damper bottoms more often and the harshness returns.
This is why Bonpora lists compression set as one of the four inspection items across its polyurethane bump stops, alongside the static stiffness curve, hardness and appearance, all under an IATF 16949 quality system. The design life statement makes the same point from the other direction: at least 80,000 km or 2 years under normal use with no cracking, no excessive permanent deformation and no stiffness loss. Permanent deformation is not a side effect of failure; it is one of the three named conditions that define the end of a PU bump stop's life.
One practical property of the test shapes everything else in this article: it is destructive. A production part cannot be compressed for 70 hours and then shipped, so the test is run on a sample from each batch, and the record is kept with the batch documentation. Every conclusion a buyer draws from set data therefore rests on sampling discipline.
Test Conditions: Deflection, Temperature and Time
A compression set result has four inputs, and changing any of them changes the output:
Deflection — how far the specimen is squeezed, usually expressed as a percentage of its original thickness. Common industry practice for elastomer set tests uses 25% deflection; some specifications call for 40% or higher, which stresses the cellular structure much harder.
Temperature — the oven temperature during the hold. A test at 23 °C near room temperature mostly measures viscoelastic recovery; a test at 70 °C accelerates the thermal and chemical relaxation that dominates underbody service.
Duration — how long the hold lasts. 24 hours and 70 hours are both common; the longer hold exposes compounds that would keep creeping in service.
Recovery and basis — how long the specimen rests before measuring, and whether the result is expressed as a percentage of the original thickness or of the applied deflection. Both conventions exist in industry documents, so the basis must be stated.
Laboratories commonly run these tests to published method standards such as ISO 815-1 or ASTM D395; the exact edition and method should be verified with the supplier. The table below shows how the same nominal part can produce very different numbers under condition sets that all appear in industry specifications. The values are illustrative, not measured data.
| Condition set | Deflection | Temperature | Duration | What it stresses | Typical use |
|---|---|---|---|---|---|
| A | 25% | 23 °C | 24 h | Viscoelastic recovery at ambient | Shelf and storage behaviour |
| B | 25% | 70 °C | 24 h | Early thermal relaxation | Quick lot comparison |
| C | 25% | 70 °C | 70 h | Sustained thermal creep | Design-life related screening |
| D | 40% | 70 °C | 70 h | Cell structure near collapse | Heavy-duty or severe profiles |
The same compound can sit comfortably inside a 10% limit under condition A and fail a 10% limit under condition D. Neither result is wrong. They answer different questions, which is why a set value without its conditions cannot be compared, quoted against, or audited.
Why 25% Beats 70 Hours as an Anchor
The title phrase compresses a rule that buyers learn the hard way: a deflection level without a duration, or a duration without a deflection level, is not an anchor. When one quotation quotes a 25% deflection figure and another quotes a 70-hour figure, neither number can be converted into the other, and the comparison is void before it starts.
If you must choose a single anchor for a passenger car PU bump stop, a mid-severity set such as 25% deflection at elevated temperature for the longer hold is the more service-relevant screen of the common options, because it reproduces sustained compression at underbody temperatures rather than storage conditions. But the defensible position is not "25% beats 70 hours". It is that the full condition set — deflection, temperature, duration, recovery time and basis — travels with every figure, and that all quotations for a programme are tested to the same condition set. Anything less turns the set report into marketing.
From Report Percentage to Millimetres of Height Loss
Buyers rarely fail at reading a percentage; they fail at converting it into something the vehicle actually does. The arithmetic is simple once the basis is fixed. Assume the report expresses set as a percentage of the original thickness, which is the more common convention for solid elastomer specimens — confirm the basis on the report itself.
Worked example, with illustrative geometry from a released drawing:
Free height of the bumper: 80.0 mm.
Fixture compresses the specimen by 25% of free height, that is 20.0 mm, and holds it for 70 hours at 70 °C.
After the agreed recovery time, the specimen measures 75.2 mm.
Set = (80.0 − 75.2) / 80.0 = 6.0%.
Expected permanent height loss on the part: 6.0% × 80.0 mm = 4.8 mm.
Now translate 4.8 mm into vehicle behaviour. If the suspension in this illustrative example has about 42 mm of usable compression travel before the stop engages, a 4.8 mm shorter stop surrenders roughly 11% of that travel: the bumper begins to work later, and the damper covers the gap alone. The engagement point moves in millimetres, but the complaint arrives as a vague "the car rides differently than it used to".
Two cautions keep this arithmetic honest. First, the bench result is an accelerated screen, not a linear prediction of road life; a 6% laboratory figure does not mean the part loses 4.8 mm in service, it means the compound and cure can hold their shape under that specific stress. Second, a 4% result at 23 °C/24 h and a 6% result at 70 °C/70 h are not subtractable figures. The workshop check is more direct: measure the free height against the released dimension, and treat height loss that does not recover after removal as excessive permanent deformation — one of the three failure conditions catalogued in Bonpora's bump stop failure analysis.
Reading a Supplier Set Report: Four Patterns
Because the test is destructive and run per batch, the value of a report lies less in the single figure than in how figures move between batches. Four patterns cover almost every situation, and each points to a different corrective direction:
| Result pattern | Interpretation | Corrective direction |
|---|---|---|
| Within limit, consistent | Process under control | No action |
| Within limit but drifting upward | Early-stage process change | Re-check cure and dosing |
| Outside limit for one batch | Isolated process excursion | Contain and re-test the lot |
| Outside limit across batches | Compound or cure design issue | Re-develop the formulation |
When you audit a supplier, ask for the last several batches of set results on the reference part, not just the passing certificate. A single in-limit number proves nothing about the process; a stable run proves the cure window, dosing and compound identity are held. A drifting trend that still passes is the most valuable data a buyer can receive, because it arrives while containment is still cheap.
Three questions expose how the supplier actually runs the test:
Which method standard and edition does the laboratory follow, and is the set basis a percentage of original thickness or of deflection?
Is the test run on a sample from every production batch, and where is the record kept?
What triggers a re-test: tooling repair, compound change, a new cure schedule, or nothing?
A supplier who answers all three with specifics is running set as a process control. A supplier who answers with a catalogue figure is running it as paperwork.
What Drives Set: Cure, Post-Cure and Compound Identity
Excess set is almost never a material accident; it is a process signature. Three levers dominate.
Cure completeness. A part can measure correctly for hardness and still carry an incomplete cure that appears later as permanent deformation. Set is the slow test that catches what the hardness reading misses, which is why cutting cure time or temperature to raise throughput shows up first as drifting set rather than as failing hardness.
Post-cure. After demoulding, which typically happens within roughly 15 to 60 minutes depending on the system and part mass, the part is nowhere near final properties. NDI systems in particular need a long post-cure, typically one to several days at elevated temperature, for the polymer network to fully develop. Skipping or shortening post-cure is a known route to drifting hardness and high set. A buyer comparing NDI and MDI quotations should treat the post-cure schedule as part of the quotation: a shorter, milder schedule is a cost saving taken out of dimensional stability.
Compound identity and system choice. MDI-based polyurethane offers a balance of resilience, tear resistance and cost for the majority of passenger car positions. NDI is selected where better retention of properties under heat and repeated cycling is required, at higher material cost and a more demanding casting process. Neither system eliminates set. Both are also adjustable: Bonpora states a working range of −40 °C to +90 °C and notes that the compound can be adjusted for special conditions, with the stiffness curve and compression set re-verified before any new version is released. A compound change without re-verification is precisely the "outside limit across batches" pattern in the table above.
The practical consequence: set performance is negotiated through process evidence — per-batch destructive records, a declared post-cure schedule, and a declared re-verification rule — not through adjectives.
A Cost Model for Excess Set
Excess set does not damage the bumper; it damages the damper's working conditions and eventually the warranty line. The mechanism is quiet: the stop engages later, the damper bottoms more often, complaints accumulate, and claims arrive against the suspension assembly rather than the rubber. The model below puts a number on it. All figures are illustrative and exist to show the arithmetic, not to quote any supplier's performance.
| Line | Supplier A | Supplier B |
|---|---|---|
| Annual volume (pieces) | 20,000 | 20,000 |
| Free height (mm) | 80.0 | 80.0 |
| Set at the agreed condition set | 5% | 9% |
| Expected height loss (mm) | 4.0 | 7.2 |
| Illustrative claim rate | 0.40% | 1.10% |
| Claims per year | 80 | 220 |
| Cost per claim (part, labour, freight) | 38.50 USD | 38.50 USD |
| Annual claim cost | 3,080.00 USD | 8,470.00 USD |
| Unit price (illustrative) | 2.10 USD | 1.86 USD |
| Annual piece-price saving | — | 4,800.00 USD |
| Net position vs Supplier A | — | −590.00 USD |
Supplier B is 0.24 USD cheaper per piece and loses 590.00 USD a year once the higher claim rate is charged against the saving. The breakeven is easy to carry into any negotiation: the claim-rate gap that exactly consumes a 0.24 USD price advantage at 20,000 pieces is 0.24 / 38.50 ≈ 0.62 percentage points. Beyond that gap, the cheaper part is the expensive one.
Two refinements strengthen the model. First, claim rates should come from the buyer's own warranty data by reference family, not from a brochure. Second, the height-loss lines make the argument physical: 7.2 mm of set on an 80 mm stop is visible on a bench, which turns the claim discussion into a measurement discussion.
Writing Compression Set into the Drawing: Field Sheet and Checklist
Everything above compresses into twelve fields. Copy them into the drawing or the purchase specification, and every quotation that arrives can be compared line by line.
| # | Field | What to write |
|---|---|---|
| 1 | Free height and tolerance | Nominal mm, with tolerance band from the released drawing |
| 2 | Test deflection | e.g. 25% of free height, stated explicitly |
| 3 | Test temperature | °C of the hold, e.g. 70 °C |
| 4 | Duration | Hours of the hold, e.g. 70 h |
| 5 | Recovery time | Minutes before measurement, agreed per method |
| 6 | Result basis | % of original thickness or % of deflection — state which |
| 7 | Method standard | Standard number and edition, verified with the supplier |
| 8 | Limit | Maximum % accepted, written as a drawing value |
| 9 | Sampling | Destructive test on a sample from each production batch |
| 10 | Records | Result kept with the batch documentation, retrievable by batch code |
| 11 | Re-test triggers | Tooling repair, compound change, cure change |
| 12 | Change control | New compound or profile re-verifies curve and set before release |
Then run this checklist before the first purchase order:
Fix one condition set for the programme and require every quotation to be tested to it.
Confirm the method standard, edition and result basis in writing, not in a brochure.
Write the set limit as a number on the drawing, with the conditions beside it.
Require per-batch destructive testing, and ask where the records live.
Ask for the last several batches of results on the reference part, and read the trend, not the single pass.
Ask for the declared post-cure schedule and demoulding window.
Ask which incoming checks verify compound identity before casting.
Agree the recovery time before measurement, so two laboratories agree.
Require the stiffness curve and the set result from the same batch sample.
For hot-climate programmes, ask how the compound adjustment is re-verified.
Tie the set limit to the warranty clause, so a claim can be settled on data.
Keep the golden sample, and re-test after any tooling or compound event.
A specification built this way survives personnel changes on both sides, because the conditions are on the paper rather than in the relationship.
Request a specification review or a sample with batch set records: Contact Bonpora.
Frequently Asked Questions
Is a lower compression set value always the better part?
Not across different test conditions. A 4% result under mild conditions can represent a worse part than a 6% result under severe conditions. Within one agreed condition set, a lower and, above all, a more consistent value indicates a compound and cure that hold their shape. Consistency between batches matters at least as much as the level.
Can I compare a 24-hour result with a 70-hour result by scaling?
No. The relationship between hold duration and remaining deformation is not a straight line, and it depends on the compound and the temperature. Scaling a short test up to a longer equivalent is a guess dressed as arithmetic. If the two quotations were tested to different durations, ask one supplier to re-run the test to the other condition set, or run both on the golden sample.
Why did hardness pass on every batch but the parts still took a set in the field?
Because hardness and set measure different things. A part can measure correctly for hardness and still carry an incomplete cure that appears later as permanent deformation. This is exactly why compression set is run as a destructive per-batch test rather than inferred from the durometer reading.
We received two batches with matching hardness but clearly different set results. What does that mean?
Read it as a process signal, not as two bad parts. Matching hardness with diverging set usually points to a cure schedule change, a dosing drift, or a compound substitution that hardness alone does not resolve. Ask for the batch records behind both results, and hold the second batch until the pattern is explained and the lot is contained or re-tested.
Does specifying an NDI compound remove compression set concerns?
No system removes the concern. NDI is selected where better retention of properties under heat and repeated cycling is needed, but it still requires complete cure and a genuine post-cure to deliver that retention. An NDI quotation with a shortened post-cure schedule can behave worse in service than a well-cured MDI part, which is why the process evidence travels with the material name.
What set limit should I write on the drawing for a passenger car bump stop?
There is no universal number that transfers between profiles, compounds and condition sets. The defensible route is to ask the supplier for batch history on the reference part under your agreed condition set, write a limit near the middle of that demonstrated distribution with a margin, and treat the limit as a drawing value that changes only through the change-control process. A limit copied from a different programme's drawing is a number without evidence.