- 1. What Shore A Hardness Measures, and What It Cannot
- 2. Where Shore A Ends and Shore D Starts
- 3. A Load Path Method for Choosing Shore A Hardness
- 4. Hardness Bands by Application
- 5. Why 85A Is Not a Soft Part
- 6. Specifying and Verifying Shore A Hardness: The Call Sheet
- 7. What a Wrong Hardness Band Costs
- 8. FAQ
- 8.1. What does 85 Shore A hardness mean for a bump stop?
- 8.2. Can I convert 90 Shore A to Shore D?
- 8.3. Why does one supplier's 80A part feel stiffer than another supplier's 85A part?
- 8.4. Should the drawing state one hardness number or a range?
- 8.5. Does hardness change with temperature in service?
- 8.6. Can hardness be checked on a part that is already fitted to a vehicle?
Shore A Hardness vs Shore D: Choose by Load Path
Shore A hardness for a bump stop is a load-path calculation, not a catalogue pick. The grade has to carry the corner load at the engagement point without over-stiffening the last part of the travel. This guide shows how to size the band, where Shore D takes over, and how to check the number delivered.

What Shore A Hardness Measures, and What It Cannot
A durometer presses a spring-loaded indentor into the material and reads how far it sinks, expressed on a 0 to 100 scale with no units. The reading is a stiffness indicator at very small strain: it says something about the compound, and nothing directly about how a finished part behaves under 40 mm of compression.
Drawings in this sector commonly cite ISO 868 or ASTM D2240, and rubber parts are also tested to ISO 7619-1. All three describe the same indentation principle with different specimen and conditioning rules, which is why the standard number belongs on the drawing next to the value rather than in a general note.
Three measurement realities decide whether a reading means anything.
The reading belongs on the finished part. The manufacturing documentation for the Bonpora jounce bumper range states that hardness is measured on the finished part, usually on a flat area rather than on a curved rib, because an unsupported reading on a thin section gives a misleadingly low figure. A bumper with a 6 mm wall and a deep waist has almost no flat area, so the location has to be agreed in writing and photographed on the first article.
Hardness identifies the compound; the curve defines the product. The same documentation draws that line explicitly: hardness describes the compound, while the static stiffness curve describes the product, because the curve is measured on the assembled bumper and therefore reflects profile, free height, hardness and cure completeness together.
It is one of four inspection items, not the acceptance test. The stated inspection set for the range is static stiffness curve, compression set, hardness and appearance, under an IATF 16949 quality system. A batch that reads correctly for hardness can still carry an incomplete cure, which shows up later as permanent deformation rather than as a low durometer figure.
That is the useful role of Shore A hardness in purchasing: the quickest measurable property of the compound, repeatable enough to compare batches, and able to catch a material mix-up before the parts reach a vehicle. It will not tell you whether the car rides correctly.
Where Shore A Ends and Shore D Starts
The A scale is built for soft and medium elastomers, the D scale for hard materials. The instruments differ in indentor geometry and spring force, so a Shore D reading is not a continuation of the Shore A number.
| Scale | Indentor | Spring force at full scale | Parts normally read on this scale | Reading trap |
|---|---|---|---|---|
| Shore A | Truncated cone, 35° with a 0.79 mm flat | About 822 g | Bump stops, bushings, dust covers, rubber mounts | Readings above about 90A lose discrimination as the spring nears the top of its travel |
| Shore D | Cone, 30° with a 0.1 mm radius tip | About 4,536 g | Rigid PU pads and spacers, hard plastic housings and collars | A soft part read on D bunches near the bottom of the scale and the number is meaningless |
The practical rule: move to the D scale once the material is harder than roughly 90 Shore A, because the A-scale spring compresses close to its limit and small differences stop reading as separate values. Durometer makers' conversion charts place 90A at about 40 to 45D, and that overlap is the only region where the two scales can be compared at all. Treat a single-number conversion as an approximate band, not an equivalence, and confirm it against the standard named on the drawing.
For a bump stop, a bushing or a dust cover, the working range stays on Shore A almost without exception. Shore D appears on the same bill of material for the rigid items around them: a hard polyurethane pad, a PA66 collar, a plastic end cap. When a buyer consolidates hardness data from several suppliers into one spreadsheet, a column that mixes 85A and 55D is not a comparable column, and the scale has to be recorded as its own field.
A Load Path Method for Choosing Shore A Hardness
Most hardness arguments in a sourcing meeting are arguments about a number nobody derived. The method below derives it from the load the part carries, the only input the vehicle supplies.
Write down the load at engagement and at full bump. Take the corner sprung mass, convert it to newtons, and add the force the suspension must carry between the moment the stop touches and the moment the suspension reaches its designed limit. This is a suspension calculation, usually available from the OE drawing or a measured curve of the original part.
Divide by the contact area. Measure the flat face that meets the spring seat or the strut body. An annular face of 58 mm outside diameter and 22 mm inside diameter gives 2,262 mm², and the load divided by that area is the average pressure the compound has to carry.
Ask for curves of the same profile at three Shore A hardness grades. The comparison only works when the geometry is held constant, because profile, wall thickness and waisting move the curve as much as the compound does. Request 75A, 80A and 85A curves in the same mould.
Choose the lowest grade that reaches the target force at the intended deflection, then check set and temperature. The lowest grade that works is normally the better choice, because it engages more progressively and transmits less harshness into the body structure.
An illustrative front corner shows the arithmetic. Sprung mass is 380 kg, so 3,728 N sits on the corner; the stop engages with 42 mm of travel left, and 4,200 N of additional force has to be carried at full bump. Average pressure on the 2,262 mm² face is 4,200 / 2,262 = 1.86 MPa. If the supplier's curves for that one profile read 2,950 N at 42 mm in 75A, 3,680 N in 80A and 4,520 N in 85A, then 80A lands within 12% of the target while 85A overshoots it by 8%. Choosing 85A "to be safe" adds 23% more force than 80A at the end of the stroke, which the driver reads as a harder arrival and which loads the top mount earlier in the event.
On the Bonpora polyurethane jounce bumpers range, that curve is inspected as one of the four stated items, which is what makes the comparison possible at all: a supplier who can only report a hardness figure cannot answer the question this method asks.
Request a specification sheet or a sample built to your corner load, and the curve comparison can be run on your geometry rather than on a catalogue profile.
Hardness Bands by Application
The table below is a starting band, not a specification. Every row assumes a progressive profile of normal proportions and a duty band that matches the vehicle.
| Band | Typical use | Load character | What goes wrong if chosen blindly |
|---|---|---|---|
| 55A to 65A | Light passenger cars, comfort-led positions, large contact faces | Low pressure, long engagement, generous travel | Bottom-out earlier on a loaded car, higher compression set over a season |
| 70A to 80A | Mainstream passenger and light commercial positions | Moderate pressure, progressive rise through the last 30 to 40 mm | Usually the safe default; still needs a curve check at the temperature target |
| 80A to 90A | Heavy vehicles, limited travel, high corner loads, loaded vans | High pressure, short engagement, steep rise | Harsher small-impact feel, more load into the top mount and body structure |
| 90A to 95A | Off-road and motorsport limit stops, short-travel applications | Very high pressure over a short distance | Edge loading and reduced conformity to a mating face that is not perfectly flat |
| 40D and above | Rigid pads, spacers and end stops, not progressive bumpers | Minimal deflection by design | No progressive behaviour at all; the part behaves like a hard spacer |
The same logic transfers to bushings, where the ranges are narrower because the part is loaded in shear as well as compression. The published comparison for suspension bushings puts natural rubber at about 45 to 75 Shore A and polyurethane at about 70 to 95 Shore A, with the note that a harder grade sharpens the response and passes more road noise into the body. A bumper and a bushing at the same nominal Shore A hardness are not doing the same job, and a purchasing rule that copies a hardness number between part families will eventually be wrong.
Why 85A Is Not a Soft Part
The sentence "85A is fairly soft, so it should be fine" is common in sourcing threads and worth dismantling: on the Shore A hardness scale, 85 sits near the top of the chassis range, and five things are being conflated.
Hardness is not stiffness. A 85A bumper with a thin waisted wall can be softer in situ than a 65A bumper with a thick, unwaisted section, because the geometry sets how much material resists the load. This is the same distinction the manufacturing documentation makes between compound and product, and it is why a curve is requested rather than a number.
The reading depends on where it was taken. A reading on a curved rib or an unsupported thin section comes out low, so a part quoted as 85A may have been measured in a place where the indentor had nothing behind it. The first article should record the measurement location, not only the result.
Dwell time changes the number. Instantaneous readings on viscoelastic materials sit higher than readings after the specified dwell, and the two conventions are not interchangeable. The drawing should name the standard and the dwell rather than leaving it to habit.
Temperature moves the reading in service. The stated working range for the on-road range is −40 °C to +90 °C, and for the off-road range −40 °C to +100 °C, noting that the compound can be adjusted for special conditions. Within those ranges a polyurethane part stiffens as it cools and softens as it heats, so an 85A part at −30 °C is not the part that was measured at 23 °C.
The conversion to Shore D is not a translation. Charts that place 85A near 30D are approximate interpolations across two different springs. A specification that says "85A or 30D" invites a supplier to choose whichever is easier to reach.
Where the material question is genuinely open, the trade-offs between elastomer families belong in a separate comparison rather than in the hardness line of a drawing; the PU and rubber comparison across twelve properties covers that ground, including where a harder grade stops helping.
Specifying and Verifying Shore A Hardness: The Call Sheet
A hardness line on a drawing usually fails for one of two reasons: a single number with no tolerance, or a value with no measurement conditions. Ten fields avoid both.
| Field | What to write | Why it matters |
|---|---|---|
| Scale | Shore A | Prevents a D-scale reading being accepted as equivalent |
| Nominal and tolerance | 80 ± 5 Shore A | A range is what production can hold; a single number is a rejection waiting to happen |
| Standard | ISO 868, ASTM D2240 or ISO 7619-1 | Fixes the specimen, conditioning and dwell rules |
| Measurement face | The flat top face, 12 mm from any edge | Curved ribs and thin sections read low |
| Minimum section under the indentor | 6 mm, stacked or supported if thinner | An unsupported reading is not a reading of the material |
| Conditioning | 23 ± 2 °C, stated stabilisation time | Polyurethane readings drift with temperature and time |
| Number of readings | Five per part, report the median | A single reading on a moulded surface scatters |
| Parts per lot | Three parts per batch, plus one retained curve coupon | Hardness screens the batch; the curve confirms the product |
| Record | Batch code, mould number, date, operator | Makes a drift traceable to a material lot or a cure change |
| Reference curve | Force at two deflections, from the first article | Gives goods-in a second, independent check |
Goods-in inspection then follows a fixed sequence, worth writing into the receiving procedure rather than left to the inspector's judgement.
Confirm the scale on the gauge matches the drawing before touching the part.
Check that the gauge is in calibration and that the indentor is undamaged.
Let the parts stabilise at 23 ± 2 °C; do not read parts straight off a cold truck.
Identify the agreed measurement face on the first part and mark it on the inspection record.
Confirm there is at least 6 mm of material, or a supported stack, under the indentor.
Take five readings across the face, spaced at least 12 mm apart and away from edges.
Record every reading, not only the average, so scatter is visible.
Compare the median with the drawing tolerance and the batch history.
Photograph the measurement location on the first article and keep it with the batch record.
Pull one part for the retained curve coupon and store it with the batch documentation.
If the median is inside tolerance but the scatter is wide, hold the lot and ask about cure and mould temperature distribution.
If the reading is outside tolerance, quarantine before sorting; a low surface reading on an otherwise correct part points at moisture, not at the compound.
What a Wrong Hardness Band Costs
The cost of a hardness error depends almost entirely on when it is discovered. The model below is illustrative, for a 20,000-piece annual programme at 1.95 USD per part, counting only costs that appear in the first quarter after discovery.
| Discovery point | What has to happen | Illustrative cost | Hidden item |
|---|---|---|---|
| Curve review, before tooling | Grade changed on paper, no hardware exists | 0 USD | One week of engineering time |
| First article, T1 | Compound adjustment, new samples, re-approval | 480 USD air freight + 16 h at 65 USD = 1,520 USD | Three weeks of programme slip |
| Goods-in, with a hardness check | Lot held, sorted, replaced, expedited | 630 USD sorting + 1,850 USD air freight = 2,480 USD | Line stop if the buffer is thin |
| In service, after 8 months | Claims, labour, returns handling, goodwill | 180 claims at 46 USD + 180 at 0.6 h and 55 USD = 14,220 USD | The part is now associated with a noise complaint |
The ratio between the first and the last row is about nine to one on visible cost alone, before any allowance for the dealer time that never reaches an invoice. The control that prevents the last row costs a gauge, a procedure and roughly twenty minutes per lot: the twelve steps above, run on three parts, plus one retained coupon for the curve comparison.
Two process signals are worth watching between lots, because they predict a problem before it becomes a rejection. A gradual drift over several weeks points at raw material or dosing drift and should trigger a re-verification. A step change that follows a new material lot should stop the lot until it is re-qualified. A part that reads low only at the surface is the classic moisture signature, and one that reads high with a brittle feel points at the isocyanate index sitting outside the target band. Shore A hardness is the screen; the curve is the decision.
FAQ
What does 85 Shore A hardness mean for a bump stop?
It sits in the upper middle of the range used for chassis bump stops, above the mainstream passenger band and below the short-travel limit stops. Whether it is right for a given position depends on the contact area and the force the part has to carry, so the number alone cannot answer the question.
Can I convert 90 Shore A to Shore D?
Published charts place 90A at roughly 40 to 45D, and that overlap is the only region where the two scales can be compared. Outside it, a converted number is an interpolation across two different instruments, so the drawing should name one scale and one standard rather than offering a choice.
Why does one supplier's 80A part feel stiffer than another supplier's 85A part?
Because the profile, the wall thickness and the cure state all move the force-deflection curve, and because the two readings may not have been taken at the same place or with the same dwell. Compare curves at the deflection you care about, not durometer figures.
Should the drawing state one hardness number or a range?
A range with a tolerance, for example 80 ± 5 Shore A. Cast polyurethane moves slightly within a specification as isocyanate index, polyol quality and cure completeness vary, and a single number turns normal variation into a rejection.
Does hardness change with temperature in service?
Yes. The stated working range for the on-road range is −40 °C to +90 °C and for the off-road range −40 °C to +100 °C, and within that span the part stiffens when cold and softens when hot. Where a position runs near the top of the range, the first-article curve should be repeated at temperature.
Can hardness be checked on a part that is already fitted to a vehicle?
Not reliably. The indentor needs a flat, supported surface, a controlled temperature and a clean face, none of which a fitted bumper offers. Free height and engagement point are the practical field checks; hardness belongs at goods-in.